Plastic Shrinkage in Injection Molding: Rates, Causes and Tool Compensation (2026)

RCRay Chan·2026-11-02·29 min read
Table of Contents

The Snapshot

  • Shrinkage is a process result, not a material constant. The datasheet value assumes a wall thickness, a flow direction, a packing pressure and a mould temperature that your part may not share.
  • Amorphous resins shrink little and evenly — roughly 0.2 to 0.8 percent, similar in every direction. Semi-crystalline resins shrink more and unevenly — commonly 1 to 2 percent or higher, and often differently along the flow than across it.
  • A range is only useful when paired with a direction. “PA6, 1.0 to 1.5 percent” is not enough information to cut a cavity; you need to know whether that figure is flow-direction, cross-flow, or an average the supplier uses for the raw stock.
  • Never cut a tight-tolerance dimension at the midpoint of a wide range. On a 100 mm part in a 0.4 to 0.7 percent band, the midpoint is 0.15 mm away from either end — three times a ±0.05 mm tolerance.
  • Glass fibre reduces shrinkage but adds directionality. Filled grades move from 1.5 percent toward 0.1 to 0.6 percent, and the difference between flow and cross-flow can become the dominant dimensional risk.
  • Packing pressure and time are the two strongest process levers. More pack means less shrinkage at the gate and a larger gradient to the far end; the goal is uniformity, not a lower average.
  • Cut steel safe. Leave material on the dimension that can be removed in one pass, and record every steel change on the tool drawing.
  • Post-mould shrinkage is real. Some semi-crystalline parts continue to change for days, so the measurement window belongs in the acceptance criteria, not in a phone call after the fact.

Shrinkage is one of those numbers everyone quotes and almost nobody checks. A toolmaker asks for a shrinkage value, the buyer forwards the resin datasheet, the number goes into a spreadsheet, the cavity is cut, and eleven weeks later a first-article report shows a dimension drifting outside tolerance on a part that “should” have been fine. The argument that follows is usually about the toolmaker’s arithmetic or the moulder’s process, when the real fault was earlier and quieter: the number in the spreadsheet was a family average, applied without direction, without a thickness context, and without asking whether the grade on the drawing was the grade in the machine.

This guide is about getting that number right, and about the second half of the problem that buyers often miss — what to do with the number once you have it. It covers what molding shrinkage actually measures, how the two polymer families behave differently, published rate tables for the common resins, what moves the value on the press, how to compensate a cavity correctly, how to agree a compensation table with the toolmaker, and where shrinkage error shows up as a visible defect.

We write tool design reviews and first-article plans for programmes delivered through a qualified mold making network under an IATF 16949-aligned quality system, and the compensation discipline below is the one we ask for on any part with a tolerance tighter than ±0.1 mm.

Table of Contents

  1. The Snapshot
  2. What Molding Shrinkage Actually Is
  3. Amorphous and Semi-Crystalline Resins Behave Differently
  4. Published Shrinkage Rates by Material
  5. Why a Range Is Not a Number
  6. Directionality: Flow Versus Cross-Flow
  7. What Moves Shrinkage on the Press
  8. Post-Mould Shrinkage and Annealing
  9. Compensating the Tool: The Arithmetic
  10. Agreeing a Compensation Table with the Toolmaker
  11. Where Shrinkage Error Shows Up as a Defect
  12. Cutting Steel Safe and Correcting at T1
  13. Frequently Asked Questions
  14. Send Us the Drawing and the Resin Grade
  15. Sources

What Molding Shrinkage Actually Is

Molding shrinkage is the percentage decrease in a dimension from the size the part has in the cavity, filled and at process temperature, to the size it has at room temperature after ejection. The word “molding” matters. The number is not a pure thermal contraction coefficient, because three separate effects are bundled into it: thermal contraction as the polymer cools, relaxation of the orientation introduced during filling, and the volumetric change that happens as the material packs and then solidifies under pressure.

That bundling is why two moulders can run the same resin and the same tool and report shrinkage values that differ by 0.2 percent. The datasheet number is measured under a specified set of conditions — a plaque of a stated thickness, a stated mould temperature, a stated packing pressure. Change the wall thickness and you change the number. Change the gate and you change the orientation field, and therefore the directional shrinkage. Change the mould temperature and you change the cooling rate, which changes crystallinity in semi-crystalline resins and therefore changes shrinkage.

For the buyer, three consequences follow immediately:

  1. A shrinkage value has no meaning without a thickness and a direction attached.
  2. The value used for tool compensation should be a decision made jointly by the toolmaker, the moulder and the buyer, recorded in a document, not a number copied from a catalogue.
  3. Because the true value will only be known after the first shots, the tool design must leave a route to correction.

That third point is the one that separates tooling that recovers from a shrinkage miss and tooling that does not. A cavity cut exactly to the nominal moulded size with no allowance on the steel has no way back except welding or a new insert. A cavity cut deliberately “heavy” on the critical dimension has a route back that costs an afternoon of machining.

Amorphous and Semi-Crystalline Resins Behave Differently

The single most useful distinction in shrinkage work is the one between amorphous and semi-crystalline polymers, because it predicts both the magnitude and the direction of the problem.

Property Amorphous resins Semi-crystalline resins
Molecular arrangement on cooling Tangled and random; no ordered regions Fold into ordered crystals as they cool
Typical shrinkage About 0.2 to 0.8 percent About 1 to 2 percent or more
Directional behaviour Roughly the same in every direction Often different along the flow than across it
Sensitivity to mould temperature Moderate Strong — crystallinity, and therefore shrinkage, depends on cooling rate
Sensitivity to packing Moderate High, especially near the gate
Common examples ABS, PC, PC/ABS, ASA, rigid PVC, PMMA, PS PP, PE, PA (nylon), POM (acetal), PBT, PEEK, PPS

Amorphous resins are easier for two reasons. Their shrinkage is smaller, so the absolute error from a wrong value is smaller, and it is roughly isotropic, so a single number can be applied to a dimension in any direction without much risk. This is why a first tool in ABS or PC is a comparatively forgiving exercise.

Semi-crystalline resins are harder for exactly the opposite reasons. Their shrinkage is larger, so an error in the value becomes a visible dimensional error, and it is anisotropic, so the same cavity can be correct along the flow and wrong across it. Add glass fibre and the anisotropy gets worse, not better: the fibre network restrains contraction along the flow direction strongly, and much less across it, so a 30 percent glass-filled grade can shrink 0.1 to 0.3 percent along the flow and several times that across it in thin sections.

The practical implication for buyers is that the material choice partly decides how much dimensional risk the project carries. If a part needs tight tolerances and a semi-crystalline resin, the tolerance and the resin are arguing with each other, and that argument should be resolved at design review, not at first article. Our material comparison guide covers the trade-offs between families, and the materials overview covers grade selection within them.

Published Shrinkage Rates by Material

The table below collects published rates for the common injection moulding resins. Treat every value as a starting point that must be confirmed against the nominated grade and the part thickness. Where sources disagree, both are shown, because the disagreement is itself informative — it shows how much the value depends on test conditions.

Resin Published shrinkage Notes
ABS 0.4 to 0.7 percent (0.5 typical; 0.6 on one published table) Amorphous; forgiving; common first-tool material
PC 0.5 to 0.7 percent Amorphous; high melt temperature; needs hot mould
PC/ABS 0.5 to 0.7 percent (0.7 on one published table) Amorphous blend; slightly higher than PC alone
PMMA (acrylic) 0.6 percent Amorphous; optical and cosmetic parts
PS (GPPS / HIPS) 0.3 to 0.6 percent (HIPS 0.4 to 0.7) Amorphous; low shrinkage
SAN / AS 0.4 to 0.7 percent Amorphous
PVC (rigid) 1.0 to 2.5 percent Wide band driven by plasticiser and formulation
POM (acetal) 2.0 to 2.5 percent (1.8 on one published table) Semi-crystalline; high, anisotropic shrinkage
PA6 (nylon) 1.0 to 1.5 percent (general injection grade 1.4 to 1.8) Semi-crystalline; moisture-sensitive
PA66 + 30% glass fibre 0.3 to 0.7 percent Filled; strongly anisotropic
PP 1.0 to 2.5 percent Semi-crystalline; strongly process-sensitive
PE (HDPE / LDPE) HDPE 1.2 to 2.5; LDPE 1.5 to 3.6 Semi-crystalline; large shrinkage
PBT 0.2 to 1.4 percent Semi-crystalline; wide band by grade
PPS about 1.0 percent Semi-crystalline; often filled in practice
PEEK about 1.2 percent Semi-crystalline, high-temperature
PPO / PPE 0.5 to 0.9 percent Amorphous-ish blend behaviour
TPE 1.0 to 2.0 percent Elastomeric; hardness-dependent

Two notes on reading that table. First, the wide bands are not sloppy reporting; they are real grade-to-grade and process-to-process variation, and the honest use of a wide band is to design the tool so that the band can be absorbed. Second, glass-filled grades need their own row, not a footnote, because the fibre content changes both magnitude and direction. Published grade-level data for glass-fibre-reinforced PA6, for example, sits in a band that runs from roughly 0.4 to 0.6 percent at 20 percent loading down to 0.1 to 0.3 percent at 40 to 50 percent loading, against 1.4 to 1.8 percent for general unfilled injection grade — a difference of more than a factor of five on the same base polymer.

Glass-fibre PA6 grade (published values) Shrinkage band
20% glass fibre 0.4 to 0.6 percent
30% glass fibre 0.3 to 0.5 percent
40% glass fibre 0.1 to 0.3 percent
50% glass fibre 0.1 to 0.3 percent
Flame-retardant, glass-fibre filled 0.2 to 0.4 percent
Halogen-free flame-retardant, unfilled 0.8 to 1.2 percent
30% mineral filled 0.6 to 0.9 percent
General unfilled injection grade 1.4 to 1.8 percent

Why a Range Is Not a Number

Here is the arithmetic that changes how buyers read datasheets. Take a 100 mm dimension in ABS with a published band of 0.4 to 0.7 percent. The midpoint of the band is 0.55 percent. If the true value turns out to be 0.4 percent, the error at 100 mm is 0.15 mm. If the true value turns out to be 0.7 percent, the error is also 0.15 mm. Both directions are outside a ±0.05 mm tolerance, and one of them is outside ±0.1 mm.

Dimension Published band Midpoint Error at the low end Error at the high end
100 mm, ABS 0.4 to 0.7 percent 0.55 percent 0.150 mm 0.150 mm
250 mm, PP 1.0 to 2.0 percent 1.50 percent 1.250 mm 1.250 mm
60 mm, POM 1.8 to 2.5 percent 2.15 percent 0.210 mm 0.210 mm

The table makes the case for two design habits. On tight-tolerance dimensions, do not expect a single shrinkage number to land the dimension; expect it to land within the band and plan a correction. And on long dimensions in high-shrinkage resins, treat the tolerance as a request that the process may not be able to honour without a steel change, so put the correction route in the tool design from the start.

Dimension type Compensation strategy
Tight tolerance (±0.05 mm and tighter) Cut safe, plan a steel correction, and agree the correction method before cutting
Medium tolerance (±0.1 to ±0.2 mm) Use the midpoint of the band, verify at T1, adjust process before adjusting steel
Generous tolerance (±0.3 mm and wider) Midpoint is fine; monitor for drift across lots rather than chasing the centre
Long dimension in a high-shrinkage resin Budget for a steel change; consider gating to minimise the flow-length spread
Glass-filled anisotropic dimension Separate flow-direction and cross-flow values; never average them into one

Directionality: Flow Versus Cross-Flow

The clearest published example of directionality is a nylon part with a 4 mm wall. The shrinkage along the vertical direction is smaller than the horizontal shrinkage, at around 70 percent of it; the horizontal range is quoted at 1.4 to 1.6 percent and the average is taken for the vertical direction. For the diameter, the large value of 1.6 percent is applied to the inner diameter and the small value of 1.4 percent to the outer diameter, deliberately, so that the tool leaves room for correction after trials.

That example contains three lessons that generalise well beyond nylon.

First, the difference between directions can be large enough to require two separate numbers on the same drawing. If the drawing says “Ø50 ±0.05” and the toolmaker applies one shrinkage value to both the bore and the outside, one of the two will be wrong.

Second, applying the larger value to the inside and the smaller to the outside is not a mistake — it is a deliberate bias that makes a correction possible. If the bore comes out undersized, the toolmaker can polish or spark out material to open it. If the bore comes out oversized, there is nothing to remove. Choosing which direction to bias is a decision about which error is recoverable.

Third, because a real part has a flow pattern, dimension by dimension the shrinkage differs. A long thin part filled from one end will shrink differently along the flow than across it, and the drawing needs to say which is which if the tolerance is tight. Our tolerance guide sets out how to write those requirements so that a toolmaker can act on them.

The practical way to handle directionality without over-engineering the drawing is to give the toolmaker a small table rather than a single value:

Dimension class Direction assumption Value source
Wall thickness Thickness direction, constrained Usually 0.2 to 0.5 percent lower than in-plane
Bore / inner diameter Cross-flow Low end of the published band
Outer diameter, boss OD Cross-flow Low end of the published band
Centre-to-centre of two features Along flow High end of the published band
Overall length along the flow path Along flow High end of the published band
Dimensions across the flow path Cross-flow Low end of the published band

That table is a starting position, not a standard. It becomes accurate for a specific part only after the first shot measurement, which is why the next section matters.

What Moves Shrinkage on the Press

Shrinkage is not fixed once the tool exists. The moulder has real influence, and knowing which levers exist is what lets a buyer distinguish a tool problem from a process problem at trial.

Variable Direction of effect on shrinkage Practical note
Wall thickness Thicker walls shrink more, and cool more slowly The strongest geometric driver; the reason a 2 mm and a 4 mm section behave differently
Packing pressure Higher pack reduces shrinkage near the gate Raises the gate-to-end gradient, which is a warp risk
Packing (hold) time Longer hold reduces shrinkage until the gate freezes Beyond gate freeze, additional time buys nothing
Melt temperature Higher melt generally raises shrinkage in semi-crystalline resins Also raises the risk of flash and degradation
Mould temperature Higher mould temperature raises crystallinity and shrinkage in semi-crystalline resins Cools slower; costs cycle time
Cooling rate Faster cooling reduces crystallinity, lowering shrinkage but raising frozen-in stress Common cause of warp rather than dimensional drift
Gate size and location Small gates and distant gates increase the pressure gradient Shrinkage becomes uneven across the part
Flow orientation Material shrinks less along the orientation direction Strongest in filled and high-draw parts
Filler content More glass or mineral filler reduces shrinkage Also raises anisotropy and abrasion
Moisture (PA, PBT, PC) Wet resin changes viscosity and dimension Dry to the resin supplier’s specification before blaming the tool

Two things are worth saying plainly about this table. The first is that packing pressure and packing time cannot fix a dimensional error caused by a wrong compensation value; they can only move the dimension within a small window and, past that window, they introduce a gradient. The second is that the moulder’s process record is evidence. When a dimension is drifting lot to lot, the first document to request is the process sheet from the run that produced good parts, followed by the drying records, because “the same settings” is a claim that is often untrue in the details that matter.

If the defect appearing is more than a dimensional drift — sink marks, short shots, flash, weld lines — the diagnosis path is different and is covered in our injection molding defects guide. A shrinkage number that is wrong produces a uniform offset; a gradient in shrinkage produces warp.

Post-Mould Shrinkage and Annealing

Not all shrinkage happens before ejection. Semi-crystalline resins in particular can continue to change dimensionally after the part leaves the tool, as residual stresses relax and crystallinity finishes developing. Parts that measured at the top of tolerance at the press can be outside tolerance a day later, and the difference is usually blamed on the tool.

The practical controls are three. Agree a measurement window and write it into the acceptance criteria — for example, all dimensional inspection performed 24 hours after moulding, at a stated temperature and humidity. Do not release parts before the window has passed on the first pilot run. And where the design allows, consider annealing as a stabilising step for parts that must hold tight tolerance over a long life: it accelerates the change rather than preventing it, so the dimension you approve is closer to the dimension your customer receives.

Annealing has costs: an extra process step, a risk of dimensional movement during the anneal, and in some resins a colour or surface change. It is not a universal answer. It is worth discussing when a part carries a tight tolerance on a semi-crystalline resin and the annual volume justifies the extra step, or when the part will see elevated service temperature that would otherwise move it in the field.

For the tool design, post-mould shrinkage means one thing: leave correction room. A cavity with a working steel allowance can absorb a 0.1 mm post-mould drift with one pass. A cavity cut exactly nominal cannot.

Compensating the Tool: The Arithmetic

Two conventions are in use, and they produce slightly different answers. The first multiplies the nominal dimension by one plus the shrinkage fraction. The second divides the nominal dimension by one minus the shrinkage fraction. The second is the mathematically correct inverse of the moulded dimension shrinking to nominal; the first is the common shop approximation.

Shrinkage Nominal × (1 + s) Nominal ÷ (1 − s) Difference on 100 mm
0.4 percent 100.400 100.402 0.002 mm
0.6 percent 100.600 100.604 0.004 mm
1.5 percent 101.500 101.523 0.023 mm
2.0 percent 102.000 102.041 0.041 mm
2.5 percent 102.500 102.564 0.064 mm

For low-shrinkage amorphous resins the difference is negligible — two microns on a 100 mm dimension at 0.6 percent, which is far below any tolerance that matters. For high-shrinkage semi-crystalline resins it is not negligible: at 2.5 percent the difference on 100 mm is 0.064 mm, which is larger than a ±0.05 mm tolerance. This is the reason the convention must be written down. Two parties using different conventions on a POM part with a tight tolerance will disagree by more than the tolerance, and both will believe they are right.

A worked illustrative example. Take a nominal outer length of 250 mm in a semi-crystalline resin with a published band of 1.0 to 2.0 percent. Using the midpoint, 1.5 percent, the multiply convention gives a cavity dimension of 253.750 mm and the divide convention gives 253.807 mm. The 0.057 mm difference is small compared with the band itself, which contributes ±1.25 mm at the extremes. The lesson is not that the convention is unimportant; it is that the convention matters less than the band, and that on a dimension like this, a steel correction should be assumed rather than hoped against.

The convention question is worth settling for a second, more practical reason: it is cheap. One line in the tool specification — “cavity dimensions calculated as nominal divided by one minus shrinkage, to four decimal places, shrinkage value per the attached table” — removes an entire category of post-trial argument.

Agreeing a Compensation Table with the Toolmaker

The deliverable that prevents most shrinkage disputes is a one-page table, attached to the tool purchase order, that lists the dimensions that matter and the value applied to each.

Column What goes in it
Dimension ID Matches the drawing, for example OD-01, BORE-03, C-C-07
Nominal and tolerance Copied from the drawing, not retyped from memory
Dimension class Bore, OD, centre-to-centre, overall length, thickness
Direction assumption Along flow or cross-flow, with a one-line justification
Shrinkage applied A single value, from a named source, with a date
Source Supplier datasheet, simulation output, or previous tool history
Cavity dimension The calculated number, to four decimals
Correction route Which direction the steel can move, and by how much
Owner and date Who agreed it, and when

Three habits make the table do its job. First, the source column must name the document and the date; “from the resin supplier” is not a source. Second, the correction route column forces the conversation about safe cutting before the steel is touched. Third, the table gets reissued whenever the resin grade changes, because a grade change is a shrinkage change.

If the part comes from a previous tool, the previous tool’s measured shrinkage is worth more than any datasheet. Ask for the old tool’s first-article report and the process sheet used to produce it; a measured value from a real production tool in the same grade is the best input a new tool can have. Where no history exists and the tolerance is tight, a flow study can provide a directional shrinkage prediction to compare against the datasheet. Our mold flow analysis guide explains how to read the shrinkage output and what it can and cannot tell you.

Where Shrinkage Error Shows Up as a Defect

Shrinkage problems rarely present as “the part is 0.2 mm small”. They present as a symptom, and the symptom points at a different root cause depending on whether the error is uniform or graded.

Symptom What shrinkage is doing Where to look first
Uniform dimensional offset, all features in the same direction Compensation value is wrong The compensation table and the resin grade, not the process
Dimensions vary between cavities Uneven packing caused by an unbalanced runner Runner balance and fill study
Dimension drifts along the flow path Shrinkage gradient from a pressure drop Gate size, packing profile, wall transitions
Warp with no dimensional error at the gate Differential shrinkage or cooling Cooling layout and wall thickness symmetry
Sink marks on a cosmetic face Local volumetric shrinkage over a thick section Rib or boss geometry, wall thickness, packing
Parts in tolerance at the press, out of tolerance next day Post-mould shrinkage Measurement window and annealing decision
Bore too small, OD too large Directional bias applied the wrong way Direction assumptions in the compensation table

The first row is the important one, because it is the only one where the answer is “the number was wrong” rather than “the process needs work”. A uniform offset across every feature is almost always a compensation error, and the fix is a steel change or, on an inner dimension, a polish-out. A graded error is a process or runner problem, and cutting steel to chase it makes the tool worse.

Cutting Steel Safe and Correcting at T1

The design decision that determines whether a shrinkage miss is a one-week fix or a six-week disaster is made before the first cut: which dimensions carry a working allowance, and in which direction.

The rule of thumb: on dimensions where material can be removed to correct — bores, slots, internal features, and any dimension where the correction is “make it bigger” — cut with a small working allowance and open it at T1. On dimensions where correction means welding or inserting, cut closer to the calculated value and rely on process adjustment plus a careful measurement window.

Correction needed Method Cost and risk
Inner dimension too small Polish, hone, spark out, or ream Low cost; the preferred direction of error
Inner dimension too large Weld and re-machine, or replace the insert High cost; avoid by cutting undersize
Outer dimension too large Grind or spark out the cavity Moderate cost; usually straightforward
Outer dimension too small Weld the cavity wall and re-machine High cost; avoid
Centre-to-centre too tight Re-position one insert or re-machine the plate Moderate to high; affects related features
Wall thickness off Re-cut the core or cavity in the affected zone Moderate; check the knock-on effect on every dependent dimension

At T1, the sequence should be: measure the agreed dimensions on a defined sample of parts from each cavity, at the agreed time after moulding; compare against the compensation table; decide whether the error is within a process window by running a small design-of-experiments on packing pressure and hold time; only then cut steel. The temptation to cut immediately after the first measurement is strong and usually wrong, because a single sample at a single process setting cannot separate a compensation error from a process setting.

Record every steel change on the tool drawing with a revision, the dimension affected, the amount removed or added, and the date. When the tool moves to a different moulder three years later, that record is the only reliable statement of what the cavity actually is. A tool without a change record is a tool whose shrinkage behaviour has to be rediscovered by trial.

For buyers who need the moulding side of this discussion rather than the tool side, our injection molding service page covers process development and first-article work, and the mold making service page covers tool design review, steel selection and gauge planning. If the question is which steel to use for the intended volume, the mold making materials guide sets out the classes and their life expectations.

Frequently Asked Questions

What is a normal shrinkage rate for plastic injection molding?

Most injection moulding resins shrink between roughly 0.4 and 2 percent, with a few grades running higher. Amorphous resins typically sit at 0.2 to 0.8 percent and semi-crystalline resins at 1 to 2 percent or more. A single “normal” number across all plastics does not exist; the family matters more than any average.

Why do semi-crystalline plastics shrink more than amorphous ones?

Because they form ordered crystalline regions as they cool, and the packing of those regions into a denser structure creates additional volume reduction beyond simple thermal contraction. That crystallisation also depends on cooling rate, which is why mould temperature has a much stronger effect on shrinkage in PP, PA and POM than in ABS or PC.

Should I use nominal × (1 + shrinkage) or nominal ÷ (1 − shrinkage)?

Both are used in industry. The divide convention is the mathematically correct inverse; the multiply convention is the common shop approximation. They differ by about 0.04 mm on a 100 mm dimension at 2 percent shrinkage, which exceeds a ±0.05 mm tolerance, so the important thing is that you and your toolmaker use the same convention and that it is written into the tool specification.

Why does my part measure in tolerance at the press and out of tolerance the next day?

Post-mould shrinkage. Semi-crystalline parts continue to relax and finish crystallising after ejection, and the change can be large enough to move a tight dimension. Agree a measurement window — often 24 hours after moulding — write it into the acceptance criteria, and consider annealing if the part must hold tolerance in service.

Can I use one shrinkage value for every dimension on the part?

Only on isotropic parts with generous tolerances. Flow direction, wall thickness and fibre content all change the value, so a competent tool design document separates at least bores, outer dimensions, centre-to-centre distances and overall length, and states the direction assumption for each.

How much does glass fibre change shrinkage?

A great deal. Published values for PA6 move from about 1.4 to 1.8 percent unfilled to 0.1 to 0.6 percent with 20 to 50 percent glass loading, with the precise figure depending on loading and grade. The fibre also increases anisotropy, so the difference between flow and cross-flow shrinkage becomes a bigger risk than the average value.

Is it better to cut steel heavy or light?

Cut in the direction that can be corrected by removing material. Bores and internal features should be cut slightly tight so they can be opened; outer cavities should be cut with an allowance so they can be ground. The error you cannot fix is the one where steel has to be added back.

How many parts should be measured at T1 to judge shrinkage?

Enough to separate part-to-part variation from a systematic offset — typically a defined sample from each cavity, measured at the agreed time after moulding, on dimensions that the compensation table lists. A single part tells you almost nothing, and a single part measured immediately after ejection tells you even less.

Do packing pressure and hold time change shrinkage?

Yes, but within a limited window. Higher packing pressure and longer hold reduce shrinkage near the gate until the gate freezes. Pushing beyond that window does not reduce the average dimension further; it increases the gate-to-end gradient, which is a warp risk rather than a dimensional fix.

Does mould temperature affect shrinkage?

Strongly, in semi-crystalline resins, because it controls cooling rate and therefore crystallinity. In amorphous resins the effect is smaller but still present. This is one reason a tool transferred to a different moulder with different cooling behaviour can produce parts that measure differently at the same nominal settings.

What is the correct shrinkage value for a new grade with no history?

Start with the resin supplier’s datasheet value for the specific grade and thickness, check whether it is flow or cross-flow, compare it against any similar grade you have produced before, and use a flow study if the tolerance is tight. Then treat the first shot as the measurement that replaces the estimate.

Why do dimensions differ between cavities in the same tool?

Usually because the runner does not fill and pack the cavities equally. A cavity that fills later is under-packed, so its parts shrink more. The fix is runner balancing, not a shrinkage value change, and a flow study is the cheapest way to see it before the tool is cut.

Can shrinkage be eliminated?

No. It can be predicted, biased and corrected, and it can be made more uniform across the part, which is what actually matters for dimensional consistency. Believing it can be eliminated is the root of most first-article arguments.

Send Us the Drawing and the Resin Grade

If you have a part with a tight tolerance and a semi-crystalline resin, the compensation table is worth agreeing before the tool is cut rather than after the first article. Send us the drawing, the nominated resin grade and the annual volume, and we will come back with a dimension-by-dimension shrinkage and compensation proposal, the correction route for each critical dimension, and a first-article plan that states when the parts will be measured.

Start at request a quote with the drawing attached, or use the contact page if you want to discuss the tolerance strategy before you commit to a design. For the tool construction side — steel, gauge planning and change records — the mold making service page has the detail, and if the question is how tight a tolerance is realistically achievable in your resin, our tolerance guide is the honest starting point.

Sources

NEXT STEP

Ready to Start Your Project?

Send us your requirements — our team responds within 24 hours. Pricing and a realistic lead time come with the reply.

RC

Written by

Ray Chan

Export Brand Manager · Injection Molding, Mold Making & DFM. Ray helps global importers and integrators source factory-direct plastic parts and tooling.

← Back to Blog