MOLDITQUICK

Mold Temperature in Injection Molding: Zones, Setpoints and Control (2026)

RCRay Chan·2026-11-04·27 min read
Table of Contents

The Snapshot

  • Mold temperature is the surface temperature of the cavity and core, not the number on the controller. The controller reads its own supply; the steel that touches the part is what decides the outcome.
  • Published setpoint bands differ by resin by a factor of three. ABS 50 to 80 °C, PMMA 40 to 90 °C, PA66 40 to 120 °C, POM 60 to 120 °C and PPS 120 to 150 °C, with a general thermoplastics band of 50 to 90 °C quoted elsewhere in the same reference set.
  • Low mold temperature freezes orientation and reduces as-molded shrink, so parts come out larger. High mold temperature gives slower cooling and more relaxation, so crystalline resins shrink more and dimensions settle more predictably.
  • The differential between core and cavity is a warpage tool. Uneven temperature makes the hot side deform toward itself after cooling; a deliberate differential can be used to cancel it.
  • Plumbing matters more than most shops admit. Circuits in series, not parallel; separate control for core and cavity; insulating plates between mold and platen; no restrictive quick-connectors on the supply.
  • Thermal equilibrium takes shots, not minutes. Published practice is to establish it over at least ten injections and to measure at many points with a thermocouple about 2 mm below the surface.
  • Residual stress is a thermal artefact. A cold mold freezes the surface layer fast, leaving compressive stress at the surface and tensile stress inside, which is documented for PC and PMMA and shows up later as stress cracking.
  • Crystalline resins keep changing after ejection. POM and PA moulded in a cold tool can continue to crystallise in service or in a paint oven and move outside tolerance well below their published heat deflection temperature.

Mold temperature is the parameter that most often gets set to make the cycle time look good, and then paid for in defects. The logic is understandable: a colder mold solidifies the part faster, cooling is the longest phase of the cycle, so a colder mold means more parts per hour. The bill arrives as rough surfaces, short shots at the end of a long flow, dimensional drift between the first and tenth shot, warpage that will not tune out, and stress cracking in the field.

The opposite error is just as common: running the tool hot because the surface finish looks better, then fighting sticking, bright spots, long cycles and post-ejection shrinkage that keeps moving the tolerance.

This guide is written as an operating manual rather than a definition. It covers what mold temperature physically is, the chain of effects it drives, the published setpoints by resin, how to split core and cavity temperatures on purpose, how to plumb and instrument the circuits so the readings mean something, and a defect matrix that maps a symptom to a mold temperature cause and a fix.

We review mold temperature as part of the process package on tooling that runs through our mold-making partners, under an IATF 16949-aligned quality system, and the review usually starts by asking where the thermocouple is rather than what setpoint is programmed.

Table of Contents

  1. The Snapshot
  2. What Mold Temperature Actually Measures
  3. The Mechanism Chain: Gloss, Fill and Dimensions
  4. Shrinkage, Crystallinity and Post-Mold Growth
  5. Internal Stress and Stress Cracking
  6. Published Setpoints by Resin
  7. Core and Cavity Differential
  8. Cooling Circuit Plumbing Rules
  9. Reaching Thermal Equilibrium
  10. Controller Selection and the Tool Data Sheet
  11. Mold Temperature Troubleshooting Matrix
  12. Mold Temperature and Tool Steel
  13. What to Ask a Molder Before Approval
  14. Frequently Asked Questions
  15. Book a Process Review
  16. Sources

What Mold Temperature Actually Measures

Mold temperature is the surface temperature of the cavity and core — the steel faces that the melt touches. That definition sounds pedantic until you compare it with what a shop usually reports, which is the setpoint on the temperature controller.

Three temperatures are in play and they are not interchangeable:

  • Controller supply temperature. The water (or oil) leaving the temperature control unit. This is the number the operator dials and the number written on the process sheet.
  • Mold surface temperature. The actual steel temperature at the cavity face, which depends on circuit layout, flow rate, steel mass, cycle time and the heat the melt brings in on every shot.
  • Melt temperature. The resin temperature at the nozzle, typically 150 to 250 °C above the mold surface, and the main source of the heat the mold has to remove.

The gap between supply and surface can be large. A circuit that is plumbed in parallel, restricted by quick-connectors and sized too small will deliver a supply temperature that looks correct while the cavity face runs several degrees cooler, and the difference shows up as a gloss band down one side of the part or a dimensional drift between cavities.

The practical consequence is that a process sheet stating “mold 60 °C” is a statement about the controller, not about the part. What determines part quality is the steel temperature at the moment the melt arrives, at the location where the part is most sensitive — which is why published practice recommends measuring at several points with a fast-response probe, or fitting a thermocouple in the mold about 2 mm from the surface.

The Mechanism Chain: Gloss, Fill and Dimensions

Mold temperature affects the part through a chain of physical events, and each link has a direction.

Fill. A cold mold removes heat from the melt on contact, thickening the frozen layer and narrowing the flow channel. The pressure needed to fill the same part rises, and the far end of a long flow path may not fill at all. A warmer mold keeps the channel open longer and lowers the pressure required.

Gloss and surface. Published practice is direct on this: the higher the mold temperature, the higher the surface gloss of the product, and vice versa. The mechanism is replication — a warmer surface lets the melt press into the steel texture before it freezes, so the texture is copied faithfully. A cold mold freezes the skin before it has fully replicated the surface, which reads as a dull or rough finish. For ABS, low mold temperature produces noticeably lower smoothness.

Colour and appearance. The exception is worth knowing: for PP with a satin finish, higher mold temperature tends to lower gloss and increase colour difference, so the relationship is not universal across resins and textures. Published guidance also notes that too high a mold temperature can cause sticking and bright spots in some areas of the part, and that too low a temperature makes the part grip the mold tightly enough to scratch on demolding, especially on textured faces.

Dimensions. The direction of the effect surprises people. A low mold surface temperature reduces in-mold shrinkage — the frozen layer thickens, molecular orientation is frozen in, and crystal growth is restricted — so the part comes out larger than it would from a hot tool. A high mold temperature gives slower cooling, more relaxation, less orientation and more crystallisation, so crystalline resins shrink more. Published guidance puts it plainly: if parts come out oversized, the mold surface temperature is often too low.

Stability. A mold that takes a long time to reach thermal equilibrium, or that has uneven heat removal in some areas, shows dimensions that drift shot after shot. Stable mold temperature reduces the fluctuation in molding shrinkage, which is what makes a tolerance capable rather than lucky.

The chain explains a common production mystery: a tool that produces in-tolerance parts at the start of a shift and out-of-tolerance parts after lunch. Nothing in the process sheet changed; the mold reached a different thermal state, or the ambient temperature in the shop moved the supply water temperature, and the shrinkage followed.

Shrinkage, Crystallinity and Post-Mold Growth

Semi-crystalline resins — POM, PA, PP, PBT, PPS — have a second stage of shrinkage that amorphous resins do not, and mold temperature controls how much of it happens inside the tool.

At a low mold temperature, the molecular chains freeze before they have arranged themselves into crystalline regions. The part ejects at one size and then continues to crystallise over hours or days, and faster if it sees heat in service, in a paint oven or in a steriliser. Because crystallisation packs the chains more tightly, the part shrinks after molding. The published warning is specific: parts molded at low temperature can deform at temperatures well below the material’s published heat deflection temperature, because the HDT was measured on a properly crystallised specimen.

The correct practice is to run near the recommended mold temperature for the resin so that crystallisation completes inside the tool. Published guidance puts it as producing close to the crystallisation temperature, ensuring adequate crystallisation during molding and avoiding post-crystallisation in a hot environment.

For amorphous resins the mechanism is different but the conclusion is similar. Amorphous parts do not crystallise, so they do not exhibit that second shrinkage stage, but they do carry frozen-in orientation and thermal stress. A cold mold freezes orientation at the surface, and that orientation relaxes later under heat, which produces the classic “the part was flat at 8 am and bowed at 4 pm” behaviour in a paint line.

The design consequence is that shrink data on a resin datasheet is a range measured under stated conditions, not a property of the material. Our plastic shrinkage guide covers the compensation side — how much steel to leave and in which direction — and the injection molding tolerances guide covers how much of the variation is absorbable in the tolerance stack.

Internal Stress and Stress Cracking

Residual stress is what happens when the outside of the part freezes before the inside. The surface layer solidifies and shrinks against the core, which is still molten and still at a higher pressure; when the core finally cools and shrinks, it pulls the already-solid skin into compression at the surface and tension in the interior.

Published observations on transparent resins make the pattern visible: in PC and PMMA, residual internal stress is compressive at the surface and tensile inside, and the surface compressive stress depends on the cooling condition — a cold mold cools the melt rapidly and creates higher residual internal stress. Polarised-light inspection of a clear part shows this as a coloured banding pattern around gates, ribs and thick sections.

The resin-specific behaviour is worth noting because it reverses between families:

  • For crystalline resins such as PP and PE, too high a mold temperature increases crystallinity and the tendency for stress cracking, so the guidance is not to run hotter than necessary.
  • For high-viscosity amorphous resins such as PC, stress cracking is related to internal stress, and a higher mold temperature reduces internal stress and the tendency to crack.

The practical test for a stressed part is simple: wipe it with a solvent or expose it to the chemical it will meet in service, and watch for crazing. A part that crazes in the lab will crack in the field, and the fix is usually a warmer mold and a slower cooling profile rather than a different resin.

Published Setpoints by Resin

The table below is the labelled portion of the published mold temperature table. It is a starting band, not a specification: the correct setpoint within the band depends on wall thickness, flow length, texture and the tolerance on the part.

Resin Published mold temperature (°C) Comment
ABS 50 to 80 Low end dulls the surface; high end improves gloss and reduces stress
PMMA 40 to 90 Optical parts run near the top of the band for stress and clarity
PA66 40 to 120 Wide band because crystallinity, not just fill, is being controlled
POM 60 to 120 Below the band, post-moulding shrinkage continues in service
PPS 120 to 150 Hot tool; needs a temperature controller rated for the duty
General thermoplastics (DFM guidance) 50 to 90 Published as a broad band, not a per-resin value

Two cautions on reading that table. First, the competitor page it comes from also lists three unlabelled rows — 10 to 60, 10 to 80 and 80 to 120 °C — whose resin attributions did not survive the published layout, so they are not usable and are marked 【待确认】 here rather than guessed. Second, a band is not a target: running a POM part at 60 °C and at 120 °C produces two different parts, and only one of them will match the shrink that was used to cut the steel.

Real programs show where the numbers land in practice. A two-shot consumer electronics housing ran PC+ABS at a 60 to 80 °C mold with a 230 to 270 °C melt, and the TPE grip at a 180 to 220 °C melt, because the overmold zone had to stay cool enough not to scorch the substrate it was bonding to. A 32-cavity POM button tool ran an 80 to 100 °C mold with a 190 to 210 °C melt, and held ±0.03 mm across every cavity — a tolerance that is only achievable because the POM was fully crystallised inside the tool rather than after it.

Core and Cavity Differential

Most shops run core and cavity at the same temperature and treat any difference as a fault. On parts with asymmetric geometry, a deliberate differential is the cheapest warpage tool available.

The mechanism: a part warps toward the hotter side as it cools, because that side stays fluid longer and shrinks more. If the part’s geometry already biases it toward one side — a deep core on one face, a flat cosmetic face on the other — a counter-bias in the cooling can cancel the geometric effect.

Published guidance approaches this structurally: control the temperature difference between the core and the cavity, between the cavity wall and the inserts, and between different regions of each half, so that the differential shrinkage of each region counteracts the orientation shrinkage differences. For symmetric parts, the guidance is the opposite — keep the temperatures consistent so cooling is balanced.

A practical method for setting the differential:

  1. Run the tool at equal core and cavity temperatures and measure flatness on the parts.
  2. Identify the direction of the bow and its magnitude.
  3. Raise the temperature on the side the part is bowing away from, in small steps, and re-measure.
  4. Stop when flatness is inside tolerance; record both temperatures on the process sheet as a pair, never as a single value.

Two cautions. A large differential raises cycle time and can create a visible gloss difference between the two faces of the part, so it is a correction of last resort rather than a substitution for correct part design. And a differential that is used to hide a wall-thickness problem will move when the wall or the gate changes, so it should be documented with the geometry revision it applies to. The geometry side of that argument is in our wall thickness guide.

Cooling Circuit Plumbing Rules

Cooling is the part of mold temperature control that determines whether the setpoint means anything. Published practice gives a compact set of rules that are routinely ignored:

Rule Published guidance What goes wrong without it
Series, not parallel Connect circuits in series rather than parallel Parallel branches flow unevenly because of resistance differences, giving a wider temperature spread than series
Separate control Use separate temperature control systems for core and cavity Cannot set a differential, cannot compensate for asymmetric geometry
Isolate the sides Isolate each side and the centre so start-up temperatures can differ Whole tool has to reach one equilibrium before running
Insulating plates Use insulating plates at the interface between mold and machine platen Heat leaks into the platens, lengthening warm-up and skewing the temperature profile
Generous bores Leave extra cross-section in the supply bores and the feed tube Pressure loss and flow starvation at the far circuits
Avoid connectors Avoid fittings that significantly obstruct flow Local restriction, uneven flow across the manifold
Pressurised water Use pressurised water where possible, with durable high-pressure pipes and manifolds Flow collapses on long circuits; hot tools cannot be run reliably
Display both temperatures Show supply and return temperature on the controller Return temperature is the only visible clue that the circuit is not removing heat

The series rule is the one that surprises people. Parallel circuits look tidier in the tool drawing, but water takes the path of least resistance, so one branch gets most of the flow and the others run nearly stagnant. The result is a mold with hot and cold zones that no single setpoint can fix, and a part with a gloss or shrink gradient across it. Series circuits force the same flow through every branch, which is why published practice prefers them.

Return temperature is the cheapest diagnostic in the plant. If supply is 60 °C and return is 61 °C, the circuit is removing almost no heat and the mold is being controlled by the ambient air rather than by the unit. A well-sized circuit on a production tool shows a meaningful supply-to-return delta, and that delta changes when a circuit blocks, which makes it a usable early warning.

Reaching Thermal Equilibrium

A mold is not at temperature when the controller says it is. It is at temperature when the heat going in from the melt equals the heat going out through the circuits, the platens and the air, and that takes shots.

Published practice is to establish thermal balance through multiple injections — generally at least ten — and then measure. The measurement method matters as much as the number:

Method Published guidance Limitation
In-mold thermocouple About 2 mm from the cavity surface Needs a sensor designed into the tool; gives the true steel temperature
Handheld high-temperature meter with fast probe Measure many points, not one side or one point Reads surface only; affected by ambient air and by timing after ejection
Controller return temperature Continuous, free, visible Indirect; reflects the circuit, not the cavity face
Part measurement Dimension and gloss after stabilisation Slowest, but the most business-relevant

The published recommendation is to establish equilibrium, measure at many points, and then adjust the setpoint to whatever produces the correct part — not to assume the datasheet band is the target. For precision parts and parts with strict appearance or safety requirements, the guidance is to run at a higher mold temperature for lower post-molding shrinkage, higher surface brightness and more consistent performance. For cost-driven parts with looser requirements, a lower temperature is acceptable if the trade-off is understood and the parts are inspected against the requirement.

A practical equilibrium protocol we use: start the tool cold, run twenty shots, record part weight, key dimensions and gloss every fifth shot, and only accept the process when three consecutive sample sets are inside the tolerance band. A tool that is still drifting at shot twenty has a cooling problem, not a setpoint problem.

Controller Selection and the Tool Data Sheet

The temperature controller is often chosen by availability rather than by duty. Four specifications decide whether it can hold a tool at temperature:

  • Temperature range and medium. A PPS tool at 120 to 150 °C needs a pressurised water unit rated for the duty, or oil. A unit sized for 90 °C will either trip or run at its limit.
  • Flow rate at pressure. The datasheet number that matters is flow at the pressure drop the mold actually presents, not free flow. Published guidance asks for the flow rate to be stated on the mold data sheet, which is the only way to check that the unit matches the circuit.
  • Heating and cooling capacity. A tool with a large steel mass and a short cycle needs more cooling capacity than the shot heat alone suggests, because it also has to reject heat leaking in from the platens.
  • Instrumentation. Supply and return temperature display, alarm on deviation, and the option to log. Without logging, a drift is invisible until the parts fail.

The mold data sheet should carry the circuit count, the bore sizes, the pressure drop at working flow, the intended medium and the target temperatures for core and cavity separately. Published guidance also suggests adding a temperature sensor in the mold to detect changes during production, which turns the tool into its own instrument.

Mold Temperature Troubleshooting Matrix

Use the symptom to find the cause before changing the setpoint, because several of these defects have the same appearance and opposite fixes.

Symptom Mold temperature cause Direction of fix
Dull or rough surface on ABS Mold surface too cold; poor replication of texture Raise mold temperature, check circuit flow and return delta
Bright spots or sticking Mold too hot locally; part adhering at ejection Lower that zone, improve cooling at the hot spot, check ejector timing
Short shot at the far end of flow Mold too cold; frozen layer chokes the channel Raise mold temperature and check the flow-length ratio
Sink marks on a thick section Uneven mold temperature; thick section cooling last Add cooling at the thick section rather than raising overall temperature
Warpage on an asymmetric part Uneven core and cavity temperatures Measure both halves; apply a controlled differential or balance the circuits
Dimensions larger than nominal Mold surface temperature too low; reduced in-mold shrink Raise mold temperature toward the published band
Dimensions drifting over a shift Mold not at thermal equilibrium, or ambient/supply drift Establish equilibrium, log supply and return, insulate the platens
Post-molding shrinkage on POM or PA Mold too cold; incomplete crystallisation Raise mold temperature toward the crystallisation range
Stress cracking or crazing in service High residual stress from fast surface cooling Raise mold temperature, slow the cooling profile, review pack pressure
Weld line weak or visible Low mold temperature at the weld location Raise temperature locally, move the weld, add a cold-slug well
Colour difference between shots Mold temperature instability Stabilise circuits, check controller capacity, log the return temperature

The matrix is not a substitute for measurement, but it prevents the most expensive mistake in process debugging: raising the mold temperature to fix a fill problem and thereby creating a sink mark, then lowering it to fix the sink and reintroducing the short shot. When the symptom moves around the part, the problem is usually distribution rather than setpoint.

Mold Temperature and Tool Steel

The steel does not set the temperature, but it decides how the tool survives it. Two interactions matter.

First, hot tools wear differently. A PPS or PEEK tool running at 120 to 150 °C holds its hardness but oxidises and loses polish faster on the cavity face, particularly around gates where shear heating adds to the mold temperature. Nitriding is the routine countermeasure: a case of roughly 0.1 to 0.3 mm at 65 to 70 HRC surface hardness raises wear resistance at gates, parting lines and slide surfaces. It does not change the thermal behaviour of the tool, and it should not be sold as a thermal fix.

Second, the steel choice and the temperature band have to be decided together. A prehardened P20 cavity at 28 to 32 HRC is fine for an ABS tool at 60 °C and for 200,000 to 300,000 shots; the same steel in a glass-filled PPS tool at 140 °C will lose its polish and its gate edges far sooner. H13 at 48 to 52 HRC after hardening and double tempering is the published answer where the combination of abrasive resin, hot tool and more than a million shots applies. S136 at 48 to 52 HRC with a mirror polish to Ra ≤0.025 µm is the choice where the surface itself is the product.

The steel and heat-treatment detail sits in our mold making materials guide, and the class definitions — Class 101 at over a million cycles and ±0.02 mm, down to Class 105 under 500 cycles — are in the production tooling guide. The temperature band for a given program should be written down next to the steel grade on the tool specification, because a tool specified for 60 °C and run at 120 °C will not deliver its stated life.

What to Ask a Molder Before Approval

Eight questions separate a controlled process from a plausible one:

  1. What is the measured mold surface temperature at the cavity and at the core, and how was it measured?
  2. How many shots were run before the measurement, and what were the part dimensions at shot five versus shot twenty?
  3. Which circuits feed the core and which feed the cavity, and are they in series or parallel?
  4. What is the supply and return temperature on each circuit at steady state?
  5. What is the differential between core and cavity, and was it set deliberately?
  6. Where are the thermocouples, and what do they read during a cycle?
  7. What is the melt temperature, and how does it relate to the published band for the resin?
  8. What is the documented cooling time, and what happens to part dimensions if it is shortened by ten percent?

Question eight is the one that reveals whether the process is understood. A molder who can answer it knows the margin; one who cannot has been running the tool at whatever settings produced acceptable parts on the day.

For parts where the mold temperature question is really a dimensional question, the injection molding tolerances guide shows how the thermal contribution sits inside the tolerance stack, and injection molding cycle time shows how cooling time trades against output.

Frequently Asked Questions

What is a normal mold temperature for injection molding?

There is no single normal. Published bands run from 40 °C at the bottom of the PMMA range to 150 °C at the top of the PPS range, with a general thermoplastics band of 50 to 90 °C. The correct value is the one that gives the required gloss, dimensions and crystallinity for that resin and that wall thickness, verified by measurement.

Should the mold temperature be higher than the melt temperature?

No. Melt temperatures are typically 150 to 250 °C above the mold surface, because the melt has to flow. Mold temperature is a heat-removal condition, not a melting condition; it is set to control cooling rate, surface replication and crystallinity.

Why do my parts come out oversized?

A low mold surface temperature is a common cause. It thickens the frozen layer, freezes molecular orientation and restricts crystal growth, all of which reduce in-mold shrinkage, so the part ejects larger. Raising the mold temperature toward the published band usually brings the dimension back.

Why does the part look dull on one side?

Uneven mold temperature across the cavity, usually caused by cooling circuits plumbed in parallel or restricted by fittings. The cold side freezes the skin before it replicates the texture, so it reads dull while the other side reads glossy. Check the supply and return temperatures on each circuit.

How long does it take for a mold to reach thermal equilibrium?

Published practice is to allow at least ten injections, and in practice a tool with a large steel mass can take longer. The test is not time but stability: part weight and key dimensions stop moving over three consecutive sample sets.

Where should the temperature sensor go?

Published guidance recommends a thermocouple in the mold about 2 mm from the cavity surface, measuring the steel the melt actually touches. A handheld meter with a fast probe is an acceptable field check if it is used at many points rather than one.

Why is the return temperature almost the same as the supply?

Because the circuit is not removing heat: flow is too low, the circuit is air-locked or blocked, or the unit is undersized for the tool. A return temperature within a degree of supply means the mold is being cooled by the surrounding air and the platens, and the setpoint is not controlling anything.

Should core and cavity run at different temperatures?

Only deliberately. For asymmetric parts a controlled differential offsets warpage; for symmetric parts equal temperatures are the published recommendation. A differential that appears by accident is a fault, and it usually indicates unbalanced circuits.

Why does POM keep shrinking after molding?

Because it has not finished crystallising. A mold below the recommended band freezes the chains before crystallisation completes, and the part continues to crystallise in storage or in service, packing tighter and shrinking. Running near the published mold temperature completes crystallisation inside the tool.

Does a hotter mold always improve surface finish?

It improves replication, which improves gloss on most resins, but the relationship is not universal. Published guidance notes that for PP with a satin finish, higher mold temperature can lower gloss and increase colour difference. The finish requirement and the resin have to be considered together.

Can mold temperature fix warpage?

Sometimes, by applying a controlled core-to-cavity differential, but only where the warpage is thermal. Warpage caused by wall-thickness variation, gate orientation or asymmetric cooling layout has to be fixed in the design. Using temperature to mask a design problem produces a process that moves when anything else changes.

How does mold temperature affect cycle time?

Cooling time is normally the longest phase of the cycle and it is set by how fast heat leaves through the steel. A hotter mold reduces the temperature difference driving heat out, so it lengthens cooling. That trade has to be made against surface quality, crystallinity and dimensional stability, not against cycle time alone.

Is a hot runner the same as a hot mold?

No. A hot runner keeps the melt in the manifold and drops at melt temperature; the mold itself still sits at its own temperature. The two systems are controlled separately, and a hot runner tool often needs a cooler cavity than a cold-runner tool because the melt arrives hotter.

What happens if the mold temperature is too high?

Published effects include thermal decomposition of the melt, sticking and bright spots on the part, longer cycles, higher crystallinity and shrinkage on crystalline resins, and increased stress-cracking tendency on PP and PE. Each of those shows up as a different defect, which is why “hotter is better for gloss” is a dangerous rule.

Book a Process Review

Send us the part drawing, the resin and the current process sheet, and we will review the mold temperature setup as a system: the published band for the resin, the core and cavity split, the circuit layout and plumbing, the equilibrium protocol and the measurement points. Where the tool is not yet built, the review happens at design stage and the cooling layout is changed on paper rather than in steel.

That review runs alongside the tool design work delivered through our mold-making service and the production process on our injection molding service. Where the geometry itself is driving the thermal problem, mold flow analysis shows what the simulation should be telling you before the steel is cut.

Request a quote through the quote form or send the process sheet and the part model through contact. If the underlying question is whether the tool can hold the tolerance at all, the injection molding tolerances guide is the better starting point.

Sources

NEXT STEP

Ready to Start Your Project?

Send us your requirements — our team responds within 24 hours. Pricing and a realistic lead time come with the reply.

RC

Written by

Ray Chan

Export Brand Manager · Injection Molding, Mold Making & DFM. Ray helps global importers and integrators source factory-direct plastic parts and tooling.